Tipi ASTM A333

Oct 19, 2023

Tipi ASTM A333

 

ASTM A333 Rekwiżiti ta' Kompożizzjoni Kimika

Kompożizzjoni Kimika ta 'ASTM A333
Element Grad 1, % Grad 3, % Grad 4, % Grad 6, % Grad 7, % Grad 8, % Grad 9, % Grad 10, % Grad 11, %
C 0.30 0.19 0.12 0.30 0.19 0.13 0.20 0.20 0.10
Mn 0.40–1.06 0.31–0.64 0.50–1.05 0.29–1.06 0.90 0.90 0.40–1.06 1.15–1.50 0.60
P 0.025 0.025 0.025 0.025 0.025 0.025 0.025 0.035 0.025
S 0.025 0.025 0.025 0.025 0.025 0.025 0.025 0.015 0.025
Si ... 0.18–0.37 0.08–0.37 0.10 min 0.13–0.32 0.13–0.32 ... 0.10–0.35 0.35
Ni ... 3.18–3.82 0.47–0.98 0.40 2.03–2.57 8.40–9.60 1.60–2.24 0.25 35.0–37.0
Cr ... ... 0.44–1.01 0.30 ... ... ... 0.15 0.50
Cu ... ... 0.40–0.75 0.40 ... ... 0.75–1.25 0.15 ...
Al ... ... 0.04–0.30 ... ... ... ... 0.06 ...
V ... ... ... 0.08 ... ... ... 0.12 ...
Cb ... ... ... 0.02 ... ... ... 0.05 ...
Mo ... ... ... 0.12 ... ... ... 0.05 0.50
Ko ... ... ... ... ... ... ... ... 0.50

 

A333 Steel Pipe

 

ASTM A333 Proprjetajiet Mekkaniċi

 

ASTM A333 Qawwa tat-tensjoni, min. Qawwa tar-Rendiment, min. Titwil %, min.
Grad Psi Mpa psi MPa Lonġitudinali Trasversali
Grad 1 55 000 380 30 000 205 35 25
Grad 3 65 000 450 35 000 240 30 20
Grad 4 60 000 415 35 000 240 30 16.5
Grad 6 60 000 415 35 000 240 30 16.5
Grad 7 65 000 450 35 000 240 30 22
Grad 8 100 000 690 75 000 515 22 ...
Grad 9 63 000 435 46 000 315 28 ...
Grad 10 80 000 550 65 000 450 22 ...
Grad 11 65 000 450 35 000 240 18 ...

 

A333 Steel Tube